Aluminum Die Casting Alloys Physical
from:network date:2009-12-11 count:267
|
Aluminum Die Casting Alloys Physical
& Mechanical Properties
Designation |
360
|
A360
|
380
|
A380
|
383
|
384
|
390
|
13
|
A13
|
43
|
218
|
|
1.Mechanical properties
|
|
Tensile strength
σb/MPa
|
300
|
320
|
320
|
320
|
310
|
330
|
320
|
300
|
290
|
230
|
310
|
|
Yield strength
σ0.2/MPa
|
170
|
170
|
160
|
160
|
150
|
170
|
250
|
140
|
130
|
100
|
190
|
|
Elongation
δ/%
|
2.5
|
3.5
|
3.5
|
3.5
|
3.5
|
2.5
|
〈1
|
2.5
|
3.5
|
9.0
|
5.0
|
|
Hardness (Brinell)
HB
|
75
|
75
|
80
|
80
|
75
|
85
|
120
|
80
|
80
|
65
|
80
|
|
Shear strength
τ/MPa
|
190
|
180
|
190
|
190
|
-
|
200
|
-
|
170
|
170
|
130
|
200
|
|
Impact strength
ακ/J
|
-
|
-
|
4
|
-
|
4
|
-
|
-
|
-
|
-
|
-
|
9
|
|
Fatigue strength
σ-1 / MPa
|
140
|
120
|
140
|
140
|
145
|
140
|
140
|
130
|
130
|
120
|
140
|
|
Modulus of elasticity
ε/GPa
|
71
|
71
|
71
|
71
|
71
|
-
|
81.3
|
71
|
-
|
71
|
-
|
|
2.Physical properties
|
|
Density
γ/(g.cm3)
|
2.63
|
2.63
|
2.74
|
2.71
|
2.74
|
2.82
|
2.73
|
2.66
|
2.66
|
2.69
|
2.57
|
|
Melting range
T/℃
|
557-
596
|
557-
596
|
540-
595
|
540-
595
|
516-
582
|
516-
582
|
510-
650
|
574-
582
|
574-
582
|
574-
632
|
535-
621
|
|
Specific heat capacity
C/(J.kg. ℃)
|
963
|
963
|
963
|
963
|
963
|
-
|
-
|
963
|
963
|
963
|
-
|
|
Thermal expansion
α(μm.m.K)
|
21.0
|
21.0
|
22.0
|
21.8
|
21.1
|
21.0
|
18.0
|
20.4
|
21.6
|
22.0
|
24.1
|
|
Thermal conductivity
λ(W.m.K)
|
113
|
113
|
96.2
|
96.2
|
96.2
|
96.2
|
134
|
121
|
121
|
142
|
96.2
|
|
Electrical conductivity
σ(%IACS)
|
30
|
29
|
27
|
23
|
23
|
22
|
27
|
31
|
31
|
37
|
24
|
|
Poisson’s ratio
μ
|
0.33
|
0.33
|
0.33
|
0.33
|
0.33
|
-
|
-
|
-
|
0.33
|
-
|
-
|
|